C87500 / CDA 875 Copper Silicon Bronze Alloys
Casting Standards :
ASTM (B Series) | B584 |
SAE (J Series) | J462 |
Federal (QQ-C- Series) | 390 |
Specification Composition :
Minimum | Maximum | |
Copper (Cu) | 79 | |
Lead (Pb) | 0.5 | |
Zinc (Zn) | 12 | 16 |
Aluminum (Al) | – | 0.5 |
Silicon (Si) | 3 | 5 |
Copper + Sum of Named Elements | 99.5 | 5 |
Specification Properties :
Heat Treat ‘F’ Denotes As Cast | Heat Treat State | Minimum |
Tensile Strength (ksi) | F | 60 |
Yield Strength (.5% extension under load) (ksi) | F | 24 |
Typical Properties :
Heat Treat State | Typical | |
Reduction of Area (%) | 20 | |
Modulus of Elasticity (ksi) | 15400 | |
Hardness (Brinell) (HB @ 500kg) | 115 | |
Machinability (% of free cutting brass) | 50 | |
Fatigue Strength (10^8 cycles) (ksi) | 22 | |
Impact Strength (Charpy) (ft-lb) | 32 | |
Compressive Strength (0.001 in. set/in.) (ksi) | 26.5 | |
Compressive Strength (0.010 in. set/in.) (ksi) | 43 | |
Compressive Strength (0.100 in. set/in.) (ksi) | 75 | |
Creep Strength (0.00001% per hour) (ksi) | 28 @ 350F | |
Melting Range (Liquidus-Solidus)(F) | 1510-1683 | |
Coefficient of Thermal Expansion (per F @ 68-400F) | 0.0000109 | |
Thermal Conductivity (Btu/sq.ft/ft./hr/F @ 68F) | 16 | |
Specific Heat (Btu/lb/F @ 68F) | 0.09 | |
Electrical Conductivity (% IACS @ 68F) | 6.7 | |
Density (lb/cu.in. @ 68F) | 0.299 | |
Pouring Temperature (Light Castings) (F) | 1900-2000 | |
Pouring Temperature (Heavy Castings) (F) | 1800-1900 | |
Patternmakers Shrinkage (in/ft) | 15/64 | |
Drossing | Low | |
Gassing | Medium | |
Fluidity | High | |
Elongation (2 inch gauge length) (%) | F | 17 |